Why is condensation a problem when welding aluminium?
If the metal is colder than the dew point of the surrounding air, water settles on the surface, just as on a cold glass of beer. At a hall temperature of 20 °C and 73 % relative humidity, a temperature difference of only 5 K is enough. The water breaks down into hydrogen in the arc and causes pores in the weld.
Production conditions therefore change with the seasons. A welding procedure that produces pore-free welds in summer can suddenly cause problems in winter or on humid spring days, without anything having changed in the wire, gas or parameters.
When does condensation form on aluminium?
Two factors are decisive: the temperature difference between air and metal, and the relative humidity. The more humid the air, the smaller the temperature difference at which water condenses.
An example: hall air at 20 °C and 60 % relative humidity has a dew point of around 12 °C. Every component and every wire spool that enters this hall colder than 12 °C will mist up. Typical situations:
- In winter, material comes into the warm hall from a lorry or an unheated store.
- The hall is heated up in the morning, while the components stay colder than the air for hours.
- In spring or when the weather changes, warm, humid air meets parts that are still at night-time temperature.
- Preheating with a fuel gas flame produces water vapour, which condenses first on the cold metal.
Thick aluminium components take a long time to reach room temperature. Condensation on aluminium is also hard to see: a thin film is barely noticeable on the bright surface.
At what humidity does water condense on the metal?
The table shows the relative humidity at which water condenses on the metal for a given temperature difference. For other values, use the Dew point calculator.
| Metal colder than the air by | Condensation at relative humidity |
|---|---|
| 1 K | from 94 % |
| 2 K | from 88 % |
| 3 K | from 83 % |
| 4 K | from 78 % |
| 5 K | from 73 % |
| 6 K | from 68 % |
| 7 K | from 64 % |
| 8 K | from 60 % |
| 10 K | from 53 % |
| 12 K | from 46 % |
| 15 K | from 37 % |
| 20 K | from 26 % |
Calculated using the Magnus formula for an air temperature of 20 °C. With cooler air the values are one to three percentage points lower, with warmer air slightly higher.
Hall air at 50 % humidity, as is usual in winter with heating, therefore tolerates a temperature difference of about 11 K. On a humid summer day at 80 %, 3 to 4 K are enough.
What does condensation do to the wire and the oxide layer?
Water on the surface does not simply dry off again. It reacts with the oxide layer to form hydrated oxide, which releases hydrogen in the arc. Every instance of condensation thus increases the hydrogen content of wire and component; more on this under Oxide layer and Solubility of hydrogen.
The Welding and Joining Institute (ISF) at RWTH Aachen University investigated this in a research project (IGF 17.524 N, 2016). Unpackaged AlSi5 and AlMg4,5Mn0,7 wires from four manufacturers were stored. The result is clear:
- Wires stored for almost a year in a warm, humid “tropical climate” (30 °C, 93 % relative humidity) or for almost two years in a workshop climate without condensation produced no pores. Their hydrogen content remained almost unchanged.
- If the wires were exposed to condensation, however, the hydrogen content rose with every cycle. From the second cycle on, pores appeared in the weld metal; after four cycles the AlMg wire could no longer be welded into a continuous bead.
- Dried-on condensate can no longer be seen on the wire later, but the pores still form.
So what matters is not how long a wire is stored, but whether condensation forms on it. Temperature changes during transport and in operation are critical: the way from a cold store into the warm hall, and the spool that stays overnight in the wire feeder of a hall that is cooling down. According to ISF, on a sultry summer day (27 °C, 75 %) it is enough to carry a poorly packed spool from a cellar at 22 °C into the workshop.
The packaging was tested too: for 54 condensation cycles, the wire in a vacuum-sealed aluminium composite bag stayed at its initial value. Moisture, by contrast, penetrated a polyethylene bag, above all to the outer windings.
How do you prevent condensation?
By letting material and wire reach the production temperature before they are opened and processed. Where that is not enough, preheating keeps the surface above the dew point.
| Situation | Remedy |
|---|---|
| Goods receipt in winter | store components and wire in the production environment for at least 24 hours; open the wire packaging only after the temperature has equalised |
| Cold components, little time | preheat until hand-warm, preferably electrically or with hot air; Preheating and interpass temperature |
| Preheating with a flame | the flame itself brings water vapour, around 31 % with propane-oxygen and around 3.6 % with acetylene-oxygen; heat until nothing condenses any more, the surface must be dry before welding |
| Storage of filler metals | in a heated storage cabinet at 30 to 40 °C |
| Opened spool | remove it from the machine at the end of work or store it protected in the cabinet; do not leave it overnight in a hall that is cooling down |
| Change in weather, humid air | measure humidity and component temperature, check the dew point, keep hall doors closed |
A simple thermo-hygrometer in the hall and a surface thermometer are enough to assess the risk before the shift starts. The Dew point calculator provides the matching dew point.
MIGAL.CO supplies its shaved aluminium wire in gas-tight vacuum packaging made of aluminium composite foil, the type of packaging that stayed tight in the ISF test. As long as it is closed, no condensation can form on the wire. That is why it pays to open it only at production temperature. All wires with data sheets: Aluminium welding wire.
Frequently asked questions
What is the dew point?
The temperature at which the air is saturated with the water vapour it contains. If air cools below this value at a cold surface, the excess water settles there. At 20 °C and 60 % relative humidity the dew point is around 12 °C.
How long does aluminium need to acclimatise before welding?
As a guideline, at least 24 hours in the production environment; for thin sheet and wire spools less is often enough, while thick components tend to need longer. The safe way is to measure the surface temperature and compare it with the dew point.
Does long storage harm aluminium welding wire?
Long storage alone hardly does, as long as the wire stays dry and no condensation forms. Temperature changes that cause condensation on the wire surface are critical.
Does it help to wipe off condensation?
Only to a limited extent. The water has already reacted with the oxide layer. It is better to warm the surface until dry and to remove the oxide shortly before welding, see Surface preparation before welding.
Further reading: articles on welding aluminium
The series follows the order of fabrication, from surface preparation to the finished weld. For an overview, see Welding aluminium: what is different from steel.
About the author
Robert Lahnsteiner, Ing., is an International Welding Engineer (IWE) and managing director of MIGAL.CO GmbH. After training in telecommunications and electronics at HTL Braunau, he spent eighteen years in welding technology at Fronius from 1983. Since 2001 he has run MIGAL.CO, the aluminium welding wire manufacturer in Landau an der Isar, together with Martin Erl. His focus is aluminium filler metals, wire manufacturing and wire feeding, and the monitoring of welding processes. Within DVS, the German Welding Society, he has served for around 30 years on technical committee FA03 “Arc welding” and chairs working group 2.4.4 “MIG welding of aluminium”.